BS 970 (Part 1):1983 637H17 Steel: Specifications & Listings

BS 970 (Part 1):1983 637H17: 637H17 is a case hardening alloy steel grade supplied to hardenability (H) requirements, specified in BS 970 Part 1:1983 (Table 10, category 2). Section three of the standard advises that category 1 steels be used for new designs and established designs whenever possible.

Category: Alloy Steel
Grade Details
GradeBS 970 (Part 1):1983 637H17
Standard BS 970 (Part 1):1983
ApplicationsCase hardening steel supplied to specified hardenability limits (end quench test, Table 10).
Equivalent / Similar Grades
Grade Standard Region Live on M-EX
BS 970 (Part 1) 637H17 BS 970 (Part 1):1991 UK No activity yet
BS 970 (Part 1) 637M17 BS 970 (Part 1):1991 UK No activity yet
IS 1570 (Part 4) 16Ni4Cr3 IS 1570 (Part 4):1988 India No activity yet
BS 970 (Part 1) 635M15 BS 970 (Part 1):1983 UK No activity yet
BS 970 (Part 1) 635H15 BS 970 (Part 1):1983 UK No activity yet
Grade ComparisonCompare With a Specific Grade →
Grade Standard Match
BS 970 (Part 1) 637M17 BS 970 (Part 1):1983 Strong Match
BS 970 (Part 1) 637H17 BS 970 (Part 1):1991 Strong Match
BS 970 (Part 1) 637M17 BS 970 (Part 1):1991 Strong Match
BS 970 (Part 3) 637M17 BS 970 (Part 3):1991 Strong Match
IS 1570 (Part 4) 16Ni4Cr3 IS 1570 (Part 4):1988 Strong Match
IS 11169 (Part 1) 16Ni4Cr3 IS 11169 (Part 1):1984 Strong Match
IS 11169 (Part 1) 16Ni4Cr3 IS 11169 (Part 1):2022 Strong Match
BS 970 (Part 1) 635M15 BS 970 (Part 1):1983 Strong Match
Matched by chemical composition and mechanical properties, not a formal equivalence claim. Always verify against the applicable standard before substitution.
Chemical Composition (%)
C Mn Cr Ni P S
0.14-0.20 0.60-0.90 0.60-1.00 0.85-1.25 <=0.035 <=0.040

More data from BS 970 (Part 1):1983

From the standard
Other composition limits
Phosphorus and sulphur
P 0.035 max, S 0.040 max, alloy steels (clause 1.7.2.1)
Residual elements: see clause 1.7.3.
Source: BS 970 (Part 1):1983, clause 1.7.2.1
Heat treatment and maximum hardness
Preheat treatment temperature (hardenability test)
930-950 deg C
Austenitizing temperature (hardenability test)
925 deg C
Maximum hardness HB, bars and billets for forging
217
Maximum hardness HB, forgings and bars for machining, normalized
217
Maximum hardness values apply when specified on the order, in the condition of delivery. Quantities not limited in Table 12 are not shown.
Source: BS 970 (Part 1):1983, Table 12
Hardenability requirements (end quench test)
Distance from quenched end (mm)HRC maxHRC min
1.54539
34537
54434
74229
94027
113724
133523
153321
203120
2530-
3029-
3528-
4028-
4527-
5026-
Rockwell C hardness at the stated distance from the quenched end in the end quench hardenability test. A dash means no value is specified. Preheat and austenitizing temperatures: see the heat treatment block.
Source: BS 970 (Part 1):1983, Table 10
Comparison with earlier editions
BS 970:1970/72 designation
637H17
BS 970:1955 En No.
None
Appendix D note 47: where a comparison is made the steels are not necessarily equivalent. 'Not listed' means the earlier edition has no entry under this designation.
Source: BS 970 (Part 1):1983, Appendix D

Active BS 970 (Part 1):1983 637H17 Listings on M-EX (For Sale)

+ Create a Listing for this grade

No active BS 970 (Part 1):1983 637H17 listings at this time.

Register for Alerts

Buyer RFQs for BS 970 (Part 1):1983 637H17

+ Post an RFQ for this grade

No open buyer requirements for BS 970 (Part 1):1983 637H17 at this time.

Register for Alerts