More data from EN 10025-2:2019
From the standard
Yield strength by thickness
8 thickness ranges
Thickness (mm) Yield strength ReH, min (MPa)
up to 16 185 over 16 to 40 175 over 40 to 63 175 over 63 to 80 175 over 80 to 100 175 over 100 to 150 165 over 150 to 200 155 over 200 to 250 145
For plate, strip and wide flats of width 600 mm or more the transverse direction applies.
Source: EN 10025-2:2019, Table 7
Tensile strength by thickness
4 thickness ranges
Thickness (mm) Tensile strength Rm (MPa)
under 3 310 to 540 3 to 100 290 to 510 over 100 to 150 280 to 500 over 150 to 250 270 to 490
Source: EN 10025-2:2019, Table 7
Elongation by thickness
5 thickness ranges
Thickness (mm) Elongation A, longitudinal, min (%) Elongation A, transverse, min (%)
3 to 40 18 16 over 40 to 63 17 15 over 63 to 100 16 14 over 100 to 150 15 13 over 150 to 250 15 13
Gauge length 5.65 times square root of cross-section area; values for thin products under 3 mm not shown.
Source: EN 10025-2:2019, Table 7 (concluded)