EN 10025-2:2019 S460K2 Steel: Specifications & Listings

EN 10025-2:2019 S460K2: S460K2: non-alloy structural steel, hot rolled flat and long products, impact tested at -20 deg C (steel number 1.0581). Specified in EN 10025-2:2019.

Category: Structural Steel
Grade Details
GradeEN 10025-2:2019 S460K2
Standard EN 10025-2:2019
ApplicationsHot rolled products of structural steels
Grade ComparisonCompare With a Specific Grade →
Grade Standard Match
EN 10025-2 S460JR EN 10025-2:2019 Strong Match
EN 10025-2 S460J0 EN 10025-2:2019 Strong Match
EN 10025-2 S460J2 EN 10025-2:2019 Strong Match
EN 10025-3 S460JR EN 10025-3:2019 Strong Match
EN 10025-3 S460 EN 10025-3:2019 Strong Match
AS/NZS 3678 Grade 450 AS/NZS 3678:2016 Strong Match
AS/NZS Grade 500 AS/NZS 3597:2008 Strong Match
EN 10025-3 S420JR EN 10025-3:2019 Close Alternative
Matched by chemical composition and mechanical properties, not a formal equivalence claim. Always verify against the applicable standard before substitution.
Chemical Composition (%)
C Si Mn P S N Cu Nb V Ti
<=0.20 <=0.55 <=1.70 <=0.030 <=0.030 <=0.025 <=0.55 <=0.05 <=0.13 <=0.05
Mechanical Properties
Tensile Strength 550-720 MPa
Yield Strength >=460 MPa
Elongation >=17%
Condition Nominal thickness up to 16 mm (tensile for 3 to 100 mm, elongation for 3 to 40 mm), longitudinal test pieces

More data from EN 10025-2:2019

From the standard
Yield strength by thickness 9 thickness ranges
Thickness (mm)Yield strength ReH, min (MPa)
up to 16460
over 16 to 40440
over 40 to 63420
over 63 to 80400
over 80 to 100390
over 100 to 150390
over 150 to 200-
over 200 to 250-
over 250 to 400-
For plate, strip and wide flats of width 600 mm or more the transverse direction applies. Long products only.
Source: EN 10025-2:2019, Table 6
Tensile strength by thickness 5 thickness ranges
Thickness (mm)Tensile strength Rm (MPa)
under 3-
3 to 100550 to 720
over 100 to 150530 to 700
over 150 to 250-
over 250 to 400-
Source: EN 10025-2:2019, Table 6
Elongation by thickness 6 thickness ranges
Thickness (mm)Elongation A, longitudinal, min (%)Elongation A, transverse, min (%)
3 to 4017-
over 40 to 6317-
over 63 to 10017-
over 100 to 15017-
over 150 to 250--
over 250 to 400--
Gauge length 5.65 times square root of cross-section area; values for thin products under 3 mm (gauge length 80 mm) not shown.
Source: EN 10025-2:2019, Table 6 (concluded)
Impact energy KV2, longitudinal 1 thickness range
Thickness (mm)Test temperature (deg C)KV2 min (J)
up to 150-2040
Longitudinal test pieces; subsized specimens reduced in proportion to area.
Source: EN 10025-2:2019, Table 8
Maximum carbon equivalent value (CEV) 5 thickness ranges
Thickness (mm)CEV, max (%)
up to 300.47
over 30 to 400.49
over 40 to 1500.49
over 150 to 250-
over 250 to 400-
Based on heat analysis.
Source: EN 10025-2:2019, Table 5

Active EN 10025-2:2019 S460K2 Listings on M-EX (For Sale)

+ Create a Listing for this grade

No active EN 10025-2:2019 S460K2 listings at this time.

Register for Alerts

Buyer RFQs for EN 10025-2:2019 S460K2

+ Post an RFQ for this grade

No open buyer requirements for EN 10025-2:2019 S460K2 at this time.

Register for Alerts