ASTM A959:2011 S40976: Ferritic stainless steel grade (UNS S40976) with the composition limits of ASTM A959-11. Carbon up to 0.030% and chromium 10.5-11.7%.
Matched by chemical composition and mechanical properties, not a formal equivalence claim. Always verify against the applicable standard before substitution.
Chemical Composition (%)
C
Cr
Mn
N
Ni
P
S
Si
Ti
<=0.030
10.5-11.7
<=1.00
<=0.040
0.75-1.00
<=0.040
<=0.030
<=1.00
>=0.05
More data from ASTM A959:2011
From the standard
Other composition limitsfrom Table 1 and its footnotes
UNS number
S40976
Metallurgical class
Ferritic grade: body-centered cubic, little or no tempered martensite, hardenable only slightly by cold working
Type
No type number is printed; the grade is identified by its UNS number only
Values
Maximum unless a range or minimum is shown; where two limits are shown for the same element in one grade the more stringent applies
Other elements (as printed)
Ti 0.05 min, Cb 10x(C+N)-0.80
These are the recommended composition limits of the A959 guide, intended for adoption by standards for stainless steel products; they are not a product specification.
Source: ASTM A959:2011, Table 1 and its footnotes
Active ASTM A959:2011 S40976 Listings on M-EX (For Sale)