BS 970 (Part 1):1983 832H13 Steel: Specifications & Listings

BS 970 (Part 1):1983 832H13: 832H13 is a case hardening alloy steel grade supplied to hardenability (H) requirements, specified in BS 970 Part 1:1983 (Table 10, category 2). Section three of the standard advises that category 1 steels be used for new designs and established designs whenever possible.

Category: Alloy Steel
Grade Details
GradeBS 970 (Part 1):1983 832H13
Standard BS 970 (Part 1):1983
ApplicationsCase hardening steel supplied to specified hardenability limits (end quench test, Table 10).
Equivalent / Similar Grades
Grade Standard Region Live on M-EX
BS 970 (Part 1) 832H13 BS 970 (Part 1):1991 UK No activity yet
BS 970 (Part 1) 832M13 BS 970 (Part 1):1991 UK No activity yet
Grade ComparisonCompare With a Specific Grade →
Grade Standard Match
BS 970 (Part 1) 832M13 BS 970 (Part 1):1983 Strong Match
BS 970 (Part 1) 832H13 BS 970 (Part 1):1991 Strong Match
BS 970 (Part 1) 832M13 BS 970 (Part 1):1991 Strong Match
BS 970 EN36C BS 970:1955 Close Alternative
IS 1570 (Part 4) 15Ni13Cr3Mo2 IS 1570 (Part 4):1988 Close Alternative
EN 10084 14NiCrMo13-4 EN 10084:2008 Close Alternative
BS 970 (Part 1) 835M15 BS 970 (Part 1):1983 Close Alternative
BS 970 (Part 1) 835H15 BS 970 (Part 1):1983 Close Alternative
Matched by chemical composition and mechanical properties, not a formal equivalence claim. Always verify against the applicable standard before substitution.
Chemical Composition (%)
C Mn Cr Mo Ni P S
0.10-0.16 0.35-0.60 0.70-1.00 0.10-0.25 3.00-3.75 <=0.035 <=0.040

More data from BS 970 (Part 1):1983

From the standard
Other composition limits
Phosphorus and sulphur
P 0.035 max, S 0.040 max, alloy steels (clause 1.7.2.1)
Residual elements: see clause 1.7.3.
Source: BS 970 (Part 1):1983, clause 1.7.2.1
Heat treatment and maximum hardness
Preheat treatment temperature (hardenability test)
880-900 deg C
Austenitizing temperature (hardenability test)
830 deg C
Maximum hardness HB, bars and billets for forging
255
Maximum hardness HB, forgings and bars for machining, sub-critically annealed
255
Maximum hardness HB, forgings and bars for machining, normalized and tempered
248
Maximum hardness values apply when specified on the order, in the condition of delivery. Quantities not limited in Table 12 are not shown.
Source: BS 970 (Part 1):1983, Table 12
Hardenability requirements (end quench test)
Distance from quenched end (mm)HRC maxHRC min
1.54437
34437
54437
74436
94434
114432
134430
154328
204226
254023
303822
353621
403521
453421
Rockwell C hardness at the stated distance from the quenched end in the end quench hardenability test. A dash means no value is specified. Preheat and austenitizing temperatures: see the heat treatment block.
Source: BS 970 (Part 1):1983, Table 10
Comparison with earlier editions
BS 970:1970/72 designation
832H13
BS 970:1955 En No.
None
Appendix D note 47: where a comparison is made the steels are not necessarily equivalent. 'Not listed' means the earlier edition has no entry under this designation.
Source: BS 970 (Part 1):1983, Appendix D

Active BS 970 (Part 1):1983 832H13 Listings on M-EX (For Sale)

+ Create a Listing for this grade

No active BS 970 (Part 1):1983 832H13 listings at this time.

Register for Alerts

Buyer RFQs for BS 970 (Part 1):1983 832H13

+ Post an RFQ for this grade

No open buyer requirements for BS 970 (Part 1):1983 832H13 at this time.

Register for Alerts